Abstract:
Shape memory and super-elastic properties of orthodontic nickel titanium wires, which are crucial for
its clinical performance are dependent on the austenitic–martensitic phase transitions in its metallic microstructure
that happen as a result of temperature or stress. The objective of this study was to compare the austenitic–martensitic
phase transitions in new, black oxide coated nickel titanium (0·016 inch, Black Diamond, NiTi) arch wires in the
‘as-received’ form, from the manufacturer and ‘retrieved form’ after two months of intraoral use. This was done to
analyse whether the new oxide coated nickel titanium wires suffered any significant loss in shape memory and super
elasticity properties at the end of two months of intra oral use, findings of which could give valuable inferences prior
to its widespread application in clinical practice.
Five arch wire samples in both groups were investigated for their austenitic–martensitic phase transitions in an
in vitro set up, using differential scanning calorimetry (DSC), (−90
◦
to 100
◦
C at a rate of 10
◦
C/min) and X-ray
diffraction (XRD) analysis (10
◦
to 90
◦
), as a function of temperature. Martensitic–austenitic thermograms showed
an intermediate rhombohedral phase in the heating cycle of both groups, but cooling cycles showed direct reversal
from austenitic to martensitic phase. Lower austenitic start (As=10·78±0·46
◦
C) and finish (Af =22·26±0·24
◦
C)
temperatures of coated wires compared to the conventional wires showed (i) ability of the wire to remain in austenitic
phase below oral temperature, that permits it to take up greater force during activation, (ii) increased springiness and (iii) consistent force delivery for an extended period of time. Statistical analysis with paired Student’s ‘t’
test did not show any significant difference in mean values of transition temperatures and enthalpies between the
two groups which proved similar shape memory and super-elastic properties at the end of intra oral use. Black
oxide coating of NiTi wires may, therefore, be effective in diversified oral conditions and may find acceptable for
re-use after sterilization. Low enthalpy values (0·92–3·59 j/g) compared to conventional ones, implied complete phase
transition at the atomic level that can improve performance of the material in activation and deactivation cycles of
NiTi wires. X-ray diffraction analysis of the two groups demonstrated predominance of austenitic phases (A, 110,
220 and 211) with complete reversibility at the atomic level. Discrete crystallographic structure and absence of multiple phases showed complete martensitic–austenitic transition, which authenticated the differential scanning calorimetric findings. This can earn acceptance for the new product in contemporary orthodontic practice with adequate
scope for indigenization